POWDER COATING PAINTING SYSTEM

Revision Date: 9/01
Process Code: Navy/Marines: ID-05-03, ID-05-04; Air Force: PA01; Army: PNT
Usage: Navy: Medium; Marines: Medium; Army: Medium; Air Force: Low
Compliance Impact: High
Alternative for: Conventional Solvent-based, Waterborne, or High Solids Painting
Applicable EPCRA Targeted Constituents: Acetone (CAS: 67-64-1), N-butyl Alcohol (CAS: 71-36-3), Lead (CAS: 7439-92-1), Methyl Ethyl Ketone (CAS: 78-93-3), Toluene (CAS: 108-88-3), Xylene (CAS: 1330-20-7)

Overview: Powder coating paint systems, also referred to as "dry painting", eliminate volatile organic compounds (VOCs), hazardous air pollutants (HAPs), and solvents, and produce superior surface finish.

There are four basic powder coating processes: electrostatic spraying, fluidized bed, electrostatic fluidized bed, and flame spray. Electrostatic spraying is the most commonly used powder application method. For all application methods, surface preparation (i.e. cleaning and conversion coating) is required to develop a good coating adhesion substrate. Characteristics of the four different powder coating application techniques are described below.

In electrostatic spraying, an electrical charge is applied to the dry powder particles while the component to be painted is electrically grounded. The charged powder and grounded workpiece create an electrostatic field that pulls the paint particles to the workpiece. The coating deposited on the workpiece retains its charge, which holds the powder to the workpiece. The coated workpiece is placed in a curing oven, where the paint particles are melted onto the surface and the charge is dissipated.

In fluidized bed, powder particles are kept in suspension by an air stream. A preheated workpiece is placed in the fluidized bed where the powder particles coming in contact with the workpiece melt and adhere to its surface. Coating thickness is dependent on the temperature and heat capacity of the workpiece and its residence time in the bed. Post heating is generally not required when applying thermoplastic powder coatings. However, post heating is required to cure thermoset powder coatings completely.

Electrostatic fluidized beds are similar in design to conventional fluidized beds, but the air stream is electrically charged as it enters the bed. The ionized air charges the powder particles as they move upward in the bed, forming a cloud of charged particles. The grounded workpiece is covered by the charged particles as it enters the chamber. No preheating of the workpiece is required. However, curing of the coating is necessary. This technology is most suitable for coating small objects with simple geometry.

The flame-spray technique was recently developed for application of thermoplastic powder coatings. The thermoplastic powder is fluidized by compressed air and fed into a flame gun where it is injected through a flame of propane, melting the powder. The molten coating particles are deposited on the workpiece, forming a film on solidification. Since no direct heating of the workpiece is required, this technique is suitable for applying coatings to most substrates. Metal, wood, rubber, and masonry can be coated successfully using this technique. This technology is also suitable for coating large or permanently-fixed objects.

The choice of powders is dependent on the end-use application and desired properties. Typically, powders are individually formulated to meet specific finishing needs. Nevertheless, powder coatings fall into two basic categories: thermoplastic and thermosetting. The choice is application dependent. Generally, thermoplastic powders are more suitable for thicker coatings, providing increased durability, while thermosetting powders are often used when comparatively thin coatings are desired, such as decorative coatings. The principal resins used in thermoplastic powders are polyethylene, polyvinyl, nylon, and fluoropolymer. Thermosetting powders use primarily epoxy, polyester, and acrylic resins.

Powder coating virtually eliminates waste streams associated with conventional painting techniques. These waste streams include air emissions, waste streams generated from air emission control equipment, and spent cleaning solvents. Powder coating also greatly reduces employee exposure, and liabilities associated with liquid coating (wet solvent) use. Because the powder is dry when sprayed, any overspray can be readily retrieved and recycled regardless of the complexity of the system This results in shorter cleanup times. In all cases, the dry powder is separated from the air stream by various vacuum and filtering methods and returned to a feed hopper for reuse. Powder efficiency (powder particles reaching the intended surface) approaches 100 percent. Other advantages over conventional spray painting include greater durability; improved corrosion resistance; and elimination of drips, runs, and bubbles.

Powder coatings are somewhat limited in their application to aerospace equipment. They typically are not used with primer systems that inhibit corrosion, but they can be successfully applied over many primed and pretreated metal substrates. If primers or pretreatments are not used, the powder coating provides protection as a barrier and prevents corrosion only as long as it is intact and undamaged. The temperatures required to cure the coating are too high for many materials used in aerospace structures (primarily aluminum); however, recently developed formulations allow baking as low as 250 degrees F which enables the use of powder coating on most materials. Powder coating can be implemented in high-production facilities with highly automated application systems or on low volume, manual batch applications. The Air Force installed the first DoD high production automated powder coating facility at Kelly AFB in 1997. In addition, there is currently an initiative to use powder coatings on aircraft landing gear at Hill AFB.


Compliance Benefit: Use of the powder coating painting systems results in the following compliance benefits:
  • Elimination of volatile organic compounds (VOCs) used as solvents in paints, which are associated with the formation of smog typically regulated by state and local air pollution control districts.
  • Elimination of hazardous air pollutants (HAPs) used as solvents in paints, which are regulated by federal, state, and local regulations including the National Emissions Standards Hazardous Air Pollutants (40 CFR 63).
  • Elimination of all SARA Title III reporting substances from coating process (by the Navy) (40 CFR 300, 355, 370, and 372; and EO 12856).
  • Reduced generation of coating waste and cleaning solvents that may need to be handled and disposed as hazardous waste under 40 CFR 260 and related sections.
  • Reduced occupational exposures that are regulated under 29 CFR 1910.

Compliance benefits include: 1) elimination of recordkeeping and reporting requirements under the Title V, NESHAP Program and SARA programs, 2) reduced administrative burden associated with hazardous waste (i.e., tracking, plans, reports, training), and 3) reduced administrative burden associated with OSHA (i.e., training and recordkeeping).

The compliance benefits listed here are only meant to be used as a general guideline and are not meant to be strictly interpreted. Actual compliance benefits will vary depending on the factors involved, e.g. the amount of workload involved.


Materials Compatibility:
Only workpieces that can be oven heated are suitable for coating by electrostatic, fluidized bed, and electrostatic fluidized bed application methods. Hence, these technologies tend to be most appropriate for relatively small, metal objects. Large standard and customized ovens are commercially available, however, for use on components of significant size.

As with all coatings, powders require a well prepared, clean surface for optimum adhesion and protection performance. Primers and pretreatments are not necessary, but additional surface preparation (for example, iron phosphate for steel, zinc phosphate for galvanized or steel substrates, and chrome phosphate for aluminum substrates) will enhance the performance of powder coatings.


Safety and Health: Powder and air mixtures can be a fire hazard when an ignition source is introduced. The concentration of powder in air must be controlled to maintain a safe working environment. Despite the absence of flammable solvents, any finely divided organic material, such as dust or powder, can form an explosive mixture in air. This is normally controlled by maintaining proper air velocity across face openings in the spray booth. In the dust collector, where it is difficult to maintain the powder concentration below the lower explosive limit, either a suppression system or a pressure relief device must be considered.

Inhalation of the powders should be avoided, as this can cause irritation to the lungs and mucous membranes. Proper personal protective equipment (PPE) should be used.

Consult your local industrial health specialist, your local health and safety personnel, and the appropriate MSDS prior to implementing this technology.


Benefits:
  • Eliminates air emissions, waste streams generated from air emission control equipment and spent cleaning solvents
  • Overspray is easily recycled for reuse.
  • Transfer efficiencies approach 100%.
  • Reduced energy requirements resulting from recirculation of powder coating spray booth air.
  • Superior finish, greater durability, improved corrosion resistance, and elimination of drips, runs and bubbles.
  • Costs of raw material (Powder) is much less expensive than Solvent Paints.
  • Clean Up (no extra solvent required for equipment maintenance).
  • Turn Around Time (Powder to cure is considerably less than Solvent Paint System).


Disadvantages:
  • Booth environment must be controlled to eliminate explosion hazards (accumulation of suspended particulate).
  • System configurations are somewhat application specific, but not severely limited.
  • Certain application limitations - such as intricate shapes and assembled components.


Economic Analysis: The following economic data and basis was provided by the Powder Coating Institute, using estimates provided by Kelly Air Force Base concerning the amount of paint used per year. It compares a conventional solvent-based coating system to a powder coating system. The conventional system includes two water wash spray booths.

Assumptions:

  • 2,500,000 ft2 painted annually
  • Cost of convention coating: $11/gal
  • Cost of powder coating: $2.35/lb
  • Surface area covered by conventional coating: 250 ft2/gal
  • Surface area covered by powder coating: 96 ft2/lb
  • Labor required for conventional coating: 5,000 hrs/year (500 ft2). This labor includes preparation time and clean up costs.
  • Powder coating system will provide a 20% saving in labor, as a result of no paint mixing requirements and reduced clean up costs.
  • Labor rate: $45/hr
  • Waste generated: 33 x 55 gal drums of waste sludge generated by the conventional coating system. 3 x 55 gal drums of waste powder generated by the powder coating system.
  • Disposal cost: $300/drum

Annual Operating Cost Comparison for Powder Coating System and Conventional Coating System

  Powder Coating Conventional Coating
Operational Costs:    
Labor: $180,000 $225,000
Material: $61,198 $110,000
Waste Disposal: $900 $10,500
Total Operational Costs: $242,098 $345,500
Total Recovered Income: $0 $0
Net Annual Cost/Benefit: -$242,098 -$345,500

Economic Analysis Summary

    Annual Savings for Powder Coating System: $103,402
    Capital Cost for Diversion Equipment/Process: $145,000
    Payback Period for Investment in Equipment/Process: < 1.5 Years

Click Here to view an Active Spreadsheet for this Economic Analysis and Enter Your Own Values. To return from the Active Spreadsheet, click the reverse arrow in the Tool Bar.


Approving Authority: Technical Orders are the source of authority for all paints used on aerospace equipment by the Air Force. The process for thermal plastic coatings and materials is contained in T.O.1-1-8, but the use of it requires approval by the engineering authority of the specific Weapon System Manager or Equipment Item Manager within the Air Force.


NSN/MSDS:
Product NSN Unit Size Cost MSDS*
ES Paint Gun 4940-01-225-3846 ea. $Local Purchase  
Fluidized Bed 3680-01-073-5290 ea. $N/A  
Flame Spray Gun 1440-01-130-5702 ea. $5,325.16  
Paint/TypeII/Red 8010-01-324-9230 50 lb. $227.50  
Paint/TypeII/Orange 8010-01-324-9227 50 lb. $227.50  


*There are multiple MSDSs for most NSNs.
The MSDS (if shown above) is only meant to serve as an example.



Points of Contact: Air Force:
Mr. Dave Ellicks
Air Force Corrosion Program Office
AFRL/MLS-OLR
325 Richmond Ray Boulevard
Robins AFB, GA 31098-1640
Phone: (478) 926-3284
DSN: 468-3284
FAX: (478) 926-6619
Civilian:
Powder Coating Institute
2121 Eisenhower Avenue
Suite 401
Alexandria, VA 22314
Phone: (703) 684-1770
FAX: (703) 684-1771
Navy:
Mr. Mark Barilla
Naval Aviation Depot
Code 4.3.4
Naval Air Station
Jacksonville, FL 32212
Phone: (904) 542-0070
or (904) 542-4519 x 129
Email:  barilliams@navair.navy.mil

Mr. Bob Frederickson
Naval Facilities Engineering Service Center, ESC 423
1100 23rd Avenue
Port Hueneme, CA 93043-4370
Phone: (805) 982-4897
DSN: 551-4889
FAX: (805) 982-4832


Vendors: This is not meant to be a complete list, as there are other manufacturers of this type of equipment.

INNOTEK Powdercoatings
3400 West Seventh Street
Big Spring,  TX   79720
Phone: (800) 753-5263 
FAX: (915) 267-1318
Service: Coating Manufacturer

Nordson Corp.
555 Jackson Street
Amherst,  OH   44001
Phone: (440) 985-4000 
FAX: (440) 985-1417
Service: Equipment Manufacturer

Sames Corporation
9201 Belmont Avenue
Franklin Park,  IL   60131
Phone: (847) 737-5970 
Service: Equipment Manufacturer

ITW Gema
4141 W. 54th Street
Indianapolis,  IN   46254
Phone: (317) 298-5000 
or (800) 628-0601
Service: Equipment Manufacturer

Morton International Powder Coatings
Box 15240
Reading,  PA   79720
Phone: (610) 775-6611 
FAX: (610) 775-6645
Service: Coating Manufacturer

Cardinal Industrial Finishes
Powder Coating Division
1329 Potrero Ave.
South El Monte,  CA   91733-3088
Phone: (626) 444-9274 
FAX: (626) 444-0382


Sources: Ms. Monique Speers, CH2M Hill (on-site Kelly AFB) conversation, January 2000.
Mr. Jeff Palmer, Powder Coating Institute, Alexandria, VA 22314
Miser, Tosko A., 1991. Powder Coatings: Chemistry and Technology, Chapter 6, Powder Coatings Application Techniques.
"Reducing Waste in Railcar Coating Operations, "Graco Equipment and Emissions Update, June 1994, pp. 8-9.
Mr. Dave Ellicks, Air Force Corrosion Prevention & Control Office, 11/99.
Mr. Vern Novstrup, NFESC, 11/99.



[Back]